The following table shows the behaviors of the Takiron FM Plate with added stress when dipping in chemicals.
The Crack and surface condition were observed after 4 weeks.
(Thickness:5.0mm)
Chemical Name Concentration
Temperatur
Added Stress
[ General purpose Grade ]
[ Heat Resistance Grade ]
Opaque
Transparent
Opaque
Transparent
FMT3331
FMET4323
FMTS3608
FMRTS4605
FMH5300
FMH5305
FMHS6650
HCL 35%
40°C
15MPa
○
△
△
△
△
○
△
30MPa
×
△
×
△
△
○
△
H2SO4 96%
40°C
15MPa
×
×
×
×
×
×
×
30MPa
×
×
×
×
×
×
×
HNO3 70%
40°C
15MPa
×
△
×
×
×
△
×
30MPa
×
×
×
×
×
×
×
HF 49%
23°C
15MPa
△
×
△
△
△
×
△
30MPa
×
×
×
△
×
×
×
H3PO4 85%
40°C
15MPa
○
○
○
○
○
○
×
30MPa
○
○
×
△
○
○
×
NH3 28%
40°C
15MPa
○
○
△
○
△
△
△
30MPa
○
○
×
△
×
△
×
H2O2 30% ※
40°C
15MPa
×
○
○
○
×
○
○
30MPa
×
○
×
×
×
×
×
HCl+H2O2+H2O 1 : 1 : 4
40°C
15MPa
○
○
○
○
○
○
○
30MPa
○
○
×
×
○
○
×
NH3+H2O2+H2O 1 : 1 : 4
40°C
15MPa
○
○
△
○
○
△
△
30MPa
○
○
×
○
○
△
×
H2SO4+H2O2 5 : 1
40°C
15MPa
×
△
×
×
×
×
×
30MPa
×
×
×
×
×
×
×
C2H5OH 100%
23°C
15MPa
○
○
×
×
○
○
×
30MPa
△
△
×
×
△
△
×
※The H2O2 was replaced with a new solution every two weeks.
○
Not Affected
△
Slightly Affected
×
Affected
The above information is correct to the best of our knowledge, but is given witout obligation on our part.
FM Listed Materals (Static Dissipative Products) Chemical Resistance
The following table shows the behaviors of the Takiron ND Series when in contact with chemicals.
Each chemical was mounted on the specimen for 24 hours.
Surface Resistivity and Appearance were observed after the contact.